Table 15. Average mechanical characteristics of K-reinforced bio-mortars obtained inthe bending and compression test.
| results | Average value | STD | results | Average value | STD | |||||
| 0 | 0 | 0 | 0 | 0 | 5.39 | / | 31.1 | / | ||
| 1 | 1 | 5 | 1 | 1 | 6.32 | 7.14 | 1.73 | 40.5 | 40.2 | 1.37 |
| 7.70 | 41.4 | |||||||||
| 7.42 | 38.7 | |||||||||
| 2 | 1 | 10 | 2 | 4 | 6.89 | 6.33 | 1.03 | 36.4 | 35.2 | 4.84 |
| 5.65 | 34.0 | |||||||||
| 6.46 | 35.4 | |||||||||
| 3 | 1 | 20 | 5 | 8 | 5.55 | 5.37 | 3.44 | 25.0 | 24.3 | 1.42 |
| 4.98 | 25.3 | |||||||||
| 5.60 | 22.7 | |||||||||
| 4 | 2 | 5 | 2 | 8 | 7.01 | 6.44 | 0.23 | 21.1 | 20.6 | 0.50 |
| 7.81 | 20.6 | |||||||||
| 6.49 | 20.1 | |||||||||
| 5 | 2 | 10 | . 5 | 1 | 4.71 | 4.63 | 1.60 | 18.9 | 18.2 | 0.91 |
| 3.95 | 17.2 | |||||||||
| 4.27 | 18.6 | |||||||||
| 6 | 2 | 20 | 1 | 4 | 2.70 | 2.53 | 1.63 | 12.2 | 14.9 | 2.53 |
| 2.53 | 17.2 | |||||||||
| 2.38 | 15.4 | |||||||||
| 7 | 5 | 5 | 5 | 4 | 5.07 | 5.54 | 0.68 | 19.0 | 20.4 | 0.36 |
| 5.23 | 20.9 | |||||||||
| 5.23 | 21.2 | |||||||||
| 8 | 5 | 10 | 1 | 8 | 3.17 | 3.60 | 1.73 | 12.60 | 12.60 | 0.13 |
| 2.76 | 13.04 | |||||||||
| 3.22 | 12.01 | |||||||||
| 9 | 5 | 20 | 2 | 1 | 3.20 | 3.20 | 1.41 | 10.7 | 10.3 | 0.52 |
| 3.17 | 10.0 | |||||||||
| 4.13 | 10.2 |